Titanum-molibdenum alloy, R0 =  5.240 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.200    6.060      38.105     1.247    6.5338      0.720         1
  1.000    2.280    7.120      85.064     1.471    7.7084      2.599         1
  1.000    2.820    8.030     118.658     1.541    8.0762      3.976         1
  1.000    5.260   10.790     297.398     1.951   10.2242     13.834         1

References:
1. A. A. Bakanova, I. P. Dudoladov, Yu. N. Sutulov, Fulfillment of additive law
   for shock-compressed alloys, Zh. Prikl. Mekh. Tekhn. Fiz. 6, 167-172 (1972)
   [in Russian] (J. Appl. Mech. Techn. Phys. 13 (1972))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g