WNZh-90 alloy, R0 = 17.100 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.650    4.810      53.463     1.156   19.7719      0.211         1
  1.000    1.270    5.700     123.787     1.287   22.0023      0.806         1
  1.000    2.120    7.060     255.939     1.429   24.4385      2.247         1
  1.000    3.520    9.080     546.543     1.633   27.9259      6.195         1

References:
1. R. F. Trunin, M. Yu. Belyakova, M. V. Zhernokletov, Yu. N. Sutulov, Shock
   compression of metallic alloys, Izv. Akad. Nauk SSSR. Fiz. Zemli 2, 99-106
   (1991) [in Russian] (Bull. Acad. Sci. USSR, Physics of the Solid Earth (1991))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g