Epoxy, fiber-polyester reinforced, R0 =  1.120 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.436    2.870       1.402     1.179    1.3206      0.095         1
  1.000    0.636    3.087       2.199     1.259    1.4106      0.202         1
  1.000    0.681    3.410       2.601     1.250    1.3995      0.232         1
  1.000    0.885    3.230       3.202     1.377    1.5427      0.392         1
  1.000    0.960    3.720       4.000     1.348    1.5096      0.461         1
  1.000    1.160    4.040       5.249     1.403    1.5711      0.673         1
  1.000    1.228    4.000       5.502     1.443    1.6162      0.754         1
  1.000    1.920    4.600       9.892     1.716    1.9224      1.843         1
  1.000    3.840    6.787      29.190     2.303    2.5794      7.373         1

References:
1. A. V. Bushman, V. P. Efremov, G. I. Kanel', I. V. Lomonosov, A. V. Utkin, V.
   E. Fortov, V. S. Yushkov, Shock compressibility and equation of state of
   orgplastic at high energy density, Khim. Fiz. 11, 410-414 (1992) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g