WNZh-95 alloy, R0 = 17.990 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.340    4.340      26.546     1.085   19.5191      0.058         1
  1.000    0.440    4.480      35.462     1.109   19.9493      0.097         1
  1.000    0.960    5.250      90.670     1.224   22.0157      0.461         1
  1.000    1.340    5.710     137.649     1.307   23.5064      0.898         1
  1.000    1.870    6.400     215.304     1.413   25.4163      1.748         1
  1.000    2.150    6.640     256.825     1.479   26.6044      2.311         1
  1.000    2.330    7.050     295.513     1.494   26.8707      2.714         1

References:
1. R. F. Trunin, M. Yu. Belyakova, M. V. Zhernokletov, Yu. N. Sutulov, Shock
   compression of metallic alloys, Izv. Akad. Nauk SSSR. Fiz. Zemli 2, 99-106
   (1991) [in Russian] (Bull. Acad. Sci. USSR, Physics of the Solid Earth (1991))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g