Steel 25CCSA, R0 =  7.770 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.860    5.180      34.614     1.199    9.3168      0.370         1
  1.000    0.960    5.610      41.846     1.206    9.3741      0.461         1
  1.000    1.370    6.050      64.402     1.293   10.0446      0.938         1
  1.000    1.650    6.440      82.564     1.344   10.4465      1.361         1
  1.000    1.840    6.890      98.505     1.364   10.6010      1.693         1
  1.000    2.500    7.790     151.321     1.473   11.4420      3.125         1
  1.000    3.070    8.720     208.006     1.543   11.9919      4.712         1

References:
1. R. F. Trunin, M. Yu. Belyakova, M. V. Zhernokletov, Yu. N. Sutulov, Shock
   compression of metallic alloys, Izv. Akad. Nauk SSSR. Fiz. Zemli 2, 99-106
   (1991) [in Russian] (Bull. Acad. Sci. USSR, Physics of the Solid Earth (1991))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g