Spodumene, R0 =  3.140 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.430    7.130       9.627     1.064    3.3415      0.092         1
  1.000    1.060    7.120      23.698     1.175    3.6892      0.562         1
  1.000    1.450    7.140      32.509     1.255    3.9402      1.051         1
  1.000    2.370    7.610      56.632     1.452    4.5602      2.808         1
  1.000    2.660    8.190      68.406     1.481    4.6504      3.538         1
  1.000    3.760    9.820     115.939     1.620    5.0883      7.069         1

References:
1. G. V. Simakov, R. F. Trunin, Minerals compression by shock waves, Izv. Akad.
   Nauk SSSR. Fiz. Zemli 2, 77-81 (1980) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g