Al-Mg alloy AMG-6, R0 =  2.640 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.660    6.280      10.942     1.117    2.9500      0.218         1
  1.000    0.770    6.440      13.091     1.136    2.9985      0.296         1
  1.000    1.140    6.950      20.917     1.196    3.1580      0.650         1
  1.000    1.470    7.410      28.757     1.247    3.2933      1.080         1
  1.000    2.750    8.840      64.179     1.452    3.8321      3.781         1
  1.000    3.360    9.570      84.890     1.541    4.0684      5.645         1
  1.000    3.760   10.170     100.952     1.587    4.1886      7.069         1
  1.000    4.100   10.760     116.466     1.616    4.2652      8.405         1
  1.000    4.290   10.770     121.977     1.662    4.3878      9.202         1
  1.000    6.050   12.770     203.963     1.900    5.0168     18.301         1

References:
1. R. F. Trunin, M. Yu. Belyakova, M. V. Zhernokletov, Yu. N. Sutulov, Shock
   compression of metallic alloys, Izv. Akad. Nauk SSSR. Fiz. Zemli 2, 99-106
   (1991) [in Russian] (Bull. Acad. Sci. USSR, Physics of the Solid Earth (1991))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g