Steel 40Cr, R0 =  7.830 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.860    5.170      34.814     1.200    9.3924      0.370         1
  1.000    0.960    5.550      41.718     1.209    9.4676      0.461         1
  1.000    1.370    6.010      64.470     1.295   10.1419      0.938         1
  1.000    1.640    6.450      82.826     1.341   10.4997      1.345         1
  1.000    1.830    6.850      98.153     1.365   10.6844      1.674         1
  1.000    2.480    7.840     152.240     1.463   11.4528      3.075         1
  1.000    3.090    8.530     206.381     1.568   12.2776      4.774         1

References:
1. R. F. Trunin, M. Yu. Belyakova, M. V. Zhernokletov, Yu. N. Sutulov, Shock
   compression of metallic alloys, Izv. Akad. Nauk SSSR. Fiz. Zemli 2, 99-106
   (1991) [in Russian] (Bull. Acad. Sci. USSR, Physics of the Solid Earth (1991))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g