Stainless steel 18C18N10T, R0 =  7.890 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.170    4.810       6.452     1.037    8.1791      0.014         1
  1.000    0.350    5.080      14.029     1.074    8.4738      0.061         1
  1.000    0.470    5.240      19.432     1.099    8.6674      0.110         1
  1.000    0.580    5.390      24.666     1.121    8.8414      0.168         1
  1.000    0.700    5.690      31.426     1.140    8.9968      0.245         1
  1.000    0.850    5.720      38.361     1.175    9.2671      0.361         1
  1.000    0.850    5.920      39.703     1.168    9.2128      0.361         1
  1.000    0.930    5.970      43.806     1.185    9.3459      0.432         1
  1.000    1.300    6.380      65.440     1.256    9.9091      0.845         1
  1.000    1.310    6.400      66.150     1.257    9.9206      0.858         1
  1.000    1.780    7.180     100.837     1.330   10.4908      1.584         1
  1.000    2.430    8.210     157.408     1.420   11.2071      2.952         1
  1.000    2.470    8.230     160.389     1.429   11.2734      3.050         1
  1.000    2.720    8.580     184.134     1.464   11.5523      3.699         1

References:
1. R. F. Trunin, M. Yu. Belyakova, M. V. Zhernokletov, Yu. N. Sutulov, Shock
   compression of metallic alloys, Izv. Akad. Nauk SSSR. Fiz. Zemli 2, 99-106
   (1991) [in Russian] (Bull. Acad. Sci. USSR, Physics of the Solid Earth (1991))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g