Sylgard, R0 =  1.037 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.369    2.028       0.776     1.222    1.2677      0.068         1
  1.000    0.401    2.073       0.862     1.240    1.2857      0.080         1
  1.000    0.440    2.383       1.087     1.226    1.2718      0.097         1
  1.000    0.461    2.426       1.160     1.235    1.2803      0.106         1
  1.000    0.465    2.265       1.092     1.258    1.3049      0.108         1
  1.000    0.469    2.364       1.150     1.247    1.2937      0.110         1
  1.000    0.472    2.251       1.102     1.265    1.3121      0.111         1
  1.000    0.551    2.492       1.424     1.284    1.3314      0.152         1
  1.000    0.556    2.423       1.397     1.298    1.3458      0.155         1
  1.000    0.802    3.142       2.613     1.343    1.3924      0.322         1
  1.000    0.812    2.922       2.461     1.385    1.4361      0.330         1
  1.000    0.993    3.604       3.711     1.380    1.4314      0.493         1
  1.000    1.003    3.405       3.542     1.418    1.4700      0.503         1
  1.000    1.156    3.525       4.226     1.488    1.5430      0.668         1
  1.000    1.290    3.708       4.960     1.533    1.5902      0.832         1
  1.000    1.462    4.271       6.475     1.520    1.5767      1.069         1
  1.000    1.481    3.989       6.126     1.591    1.6494      1.097         1
  1.000    1.792    4.790       8.901     1.598    1.6568      1.606         1
  1.000    1.800    4.688       8.751     1.623    1.6833      1.620         1
  1.000    2.555    5.613      14.872     1.836    1.9034      3.264         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g