HMX-40 wt% TATB-10 wt% Kel F 800, R0 =  1.912 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.554    3.683       3.901     1.177    2.2505      0.153         1
  1.000    0.811    4.062       6.299     1.249    2.3890      0.329         1
  1.000    0.831    4.336       6.889     1.237    2.3653      0.345         1
  1.000    0.883    4.237       7.153     1.263    2.4154      0.390         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g