Mahogany, Honduras, R0 =  0.412 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.153    1.965       0.934     2.420    0.9970      0.665         1
  1.000    1.687    2.386       1.658     3.413    1.4063      1.423         1
  1.000    1.690    2.361       1.644     3.519    1.4497      1.428         1
  1.000    2.159    3.331       2.963     2.842    1.1710      2.331         1
  1.000    2.259    3.274       3.047     3.226    1.3290      2.552         1
  1.000    2.964    4.383       5.352     3.089    1.2726      4.393         1
  1.000    3.089    4.572       5.819     3.083    1.2702      4.771         1
  1.000    3.799    5.463       8.551     3.283    1.3526      7.216         1
  1.000    4.046    5.854       9.758     3.238    1.3340      8.185         1
  1.000    4.230    6.121      10.668     3.237    1.3336      8.947         1
  1.000    4.443    6.357      11.637     3.321    1.3684      9.870         1
  1.000    4.636    6.699      12.795     3.247    1.3379     10.746         1
  1.000    5.008    7.028      14.501     3.479    1.4334     12.540         1
  1.000    5.046    7.081      14.721     3.480    1.4336     12.731         1
  1.000    5.305    7.311      15.979     3.645    1.5016     14.072         1
  1.000    5.403    7.338      16.335     3.792    1.5624     14.596         1
  1.000    5.415    7.866      17.549     3.209    1.3222     14.661         1
  1.000    5.680    7.924      18.544     3.531    1.4549     16.131         1
  1.000    5.859    8.096      19.543     3.619    1.4911     17.164         1
  1.000    5.908    8.226      20.023     3.549    1.4621     17.452         1
  1.000    6.433    8.778      23.265     3.743    1.5422     20.692         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g