Cerium oxide, R0 =  1.133 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.925    2.480       5.409     4.468    5.0628      1.853    1    1
  1.000    2.783    3.413      10.762     5.417    6.1380      3.873    1    1
  1.000    3.126    4.016      14.224     4.512    5.1125      4.886    1    1
  1.000    3.552    4.780      19.237     3.893    4.4102      6.308    1    1
  1.000    3.909    5.011      22.193     4.547    5.1520      7.640    1    1
  1.000    4.099    4.907      22.789     6.073    6.8807      8.401    1    1
  1.000    5.437    6.701      41.279     5.301    6.0065     14.781    1    1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Remarks:
1. Powdered, unpressed

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g