Kyanite, ceramic, R0 =  3.645 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.537    8.682      48.640     1.215    4.4291      1.181         1
  1.000    2.745    9.364      93.692     1.415    5.1566      3.768         1
  1.000    2.957   10.030     108.106     1.418    5.1689      4.372         1
  1.000    3.220   10.342     121.383     1.452    5.2930      5.184         1
  1.248    0.608    7.107      12.622     0.876    3.1943      0.185         1
  1.248    0.847    6.935      17.158     0.913    3.3274      0.359         1
  1.248    1.157    6.785      22.931     0.966    3.5215      0.669         1
  1.248    1.691    6.708      33.134     1.071    3.9055      1.430         1
  1.248    1.882    6.710      36.887     1.114    4.0596      1.771         1
  1.248    2.066    6.568      39.637     1.169    4.2615      2.134         1
  1.248    2.359    6.576      45.313     1.250    4.5550      2.782         1
  1.248    2.591    7.095      53.697     1.262    4.6014      3.357         1
  1.248    2.923    7.549      64.454     1.308    4.7667      4.272         1
  1.248    3.217    8.128      76.378     1.326    4.8344      5.175         1
  1.248    3.383    8.558      84.568     1.325    4.8305      5.722         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g