Cobalt-nickel alloy, R0 =  8.810 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.450    5.240      20.774     1.094    9.6377      0.101         1
  1.000    0.460    5.020      20.344     1.101    9.6987      0.106         1
  1.000    0.570    5.500      27.619     1.116    9.8286      0.162         1
  1.000    1.240    6.320      69.042     1.244   10.9605      0.769         1
  1.000    1.720    6.910     104.709     1.331   11.7297      1.479         1
  1.000    2.350    7.960     164.800     1.419   12.5005      2.761         1
  1.000    2.680    8.390     198.095     1.469   12.9450      3.591         1

References:
1. R. F. Trunin, M. Yu. Belyakova, M. V. Zhernokletov, Yu. N. Sutulov, Shock
   compression of metallic alloys, Izv. Akad. Nauk SSSR. Fiz. Zemli 2, 99-106
   (1991) [in Russian] (Bull. Acad. Sci. USSR, Physics of the Solid Earth (1991))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g