Zirconium dioxide, R0 =  4.512 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    4.428       0.000     1.000    4.5120      0.000         1
  1.000    1.622    4.864      35.597     1.500    6.7694      1.315         1
  1.000    1.736    5.219      40.880     1.498    6.7609      1.507         1
  1.000    1.825    5.511      45.380     1.495    6.7460      1.665         1
  1.000    2.113    5.493      52.370     1.625    7.3327      2.232         1
  1.000    2.299    6.305      65.402     1.574    7.1014      2.643         1
  1.000    2.477    6.854      76.602     1.566    7.0654      3.068         1
  1.000    2.797    7.156      90.309     1.642    7.4072      3.912         1
  1.000    2.994    7.436     100.452     1.674    7.5532      4.482         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g