Gold-germanium(5.8) alloy, R0 = 16.851 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    2.955       0.000     1.000   16.8510      0.000         1
  1.000    0.290    3.230      15.784     1.099   18.5132      0.042         1
  1.000    0.425    3.294      23.591     1.148   19.3472      0.090         1
  1.000    0.602    3.609      36.611     1.200   20.2246      0.181         1
  1.000    0.885    4.187      62.441     1.268   21.3674      0.392         1
  1.000    1.286    4.865     105.427     1.359   22.9059      0.827         1
  1.000    1.803    5.715     173.635     1.461   24.6175      1.625         1
  1.000    2.086    6.140     215.828     1.515   25.5217      2.176         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g