Gold-germanium(7.9) alloy, R0 = 16.111 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.487    3.270      25.657     1.175   18.9303      0.119         1
  1.000    0.488    3.271      25.717     1.175   18.9361      0.119         1
  1.000    0.599    3.508      33.854     1.206   19.4285      0.179         1
  1.000    1.101    4.442      78.793     1.330   21.4203      0.606         1
  1.000    1.274    4.707      96.613     1.371   22.0899      0.812         1
  1.000    1.542    5.255     130.551     1.415   22.8019      1.189         1
  1.000    1.809    5.661     164.989     1.470   23.6771      1.636         1
  1.000    1.819    5.629     164.963     1.477   23.8028      1.654         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g