Gold-lead(33.5) alloy, R0 = 16.032 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    2.522       0.000     1.000   16.0320      0.000         1
  1.000    0.471    3.277      24.745     1.168   18.7230      0.111         1
  1.000    0.879    3.844      54.170     1.296   20.7848      0.386         1
  1.000    1.877    5.503     165.597     1.518   24.3310      1.762         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g