Gold-lead(20.6) alloy, R0 = 17.025 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    2.644       0.000     1.000   17.0250      0.000         1
  1.000    0.448    3.395      25.894     1.152   19.6131      0.100         1
  1.000    0.840    3.966      56.718     1.269   21.5999      0.353         1
  1.000    1.816    5.555     171.746     1.486   25.2939      1.649         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g