Iron, cast, R0 =  7.174 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.319    4.909      11.234     1.069    7.6726      0.051         1
  1.000    0.577    4.997      20.685     1.131    8.1105      0.166         1
  1.000    0.760    4.917      26.809     1.183    8.4856      0.289         1
  1.000    1.111    5.445      43.398     1.256    9.0130      0.617         1
  1.000    1.196    5.642      48.409     1.269    9.1038      0.715         1
  1.000    1.797    6.620      85.343     1.373    9.8470      1.615         1
  1.000    1.883    6.889      93.061     1.376    9.8725      1.773         1
  1.000    1.939    7.044      97.985     1.380    9.8989      1.880         1
  1.000    2.055    7.163     105.601     1.402   10.0602      2.112         1
  1.000    2.285    7.518     123.240     1.437   10.3065      2.611         1
  1.000    2.572    7.987     147.372     1.475   10.5815      3.308         1
  1.000    2.799    8.311     166.885     1.508   10.8170      3.917         1
  1.000    2.993    8.767     188.243     1.518   10.8927      4.479         1
  1.000    3.020    8.618     186.713     1.539   11.0442      4.560         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g