Iron-nickel(10.0) alloy, R0 =  7.886 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.003    1.020    5.350      42.892     1.231    9.7115      0.520         1
  1.003    1.710    6.460      86.826     1.356   10.6896      1.462         1
  1.003    2.830    8.320     185.069     1.510   11.9117      4.004         1
  1.003    4.590   10.990     396.491     1.712   13.4971     10.534         1
  1.000    0.000    4.447       0.000     1.000    7.8860      0.000         2
  1.000    1.038    5.386      44.088     1.239    9.7686      0.539         2
  1.000    1.090    5.411      46.512     1.252    9.8753      0.594         2
  1.000    1.598    6.381      80.412     1.334   10.5207      1.277         2
  1.000    1.626    6.473      83.001     1.335   10.5315      1.322         2
  1.000    1.801    6.791      96.451     1.361   10.7322      1.622         2
  1.000    2.380    7.707     144.650     1.447   11.4093      2.832         2
  1.000    2.541    8.001     160.327     1.465   11.5560      3.228         2
  1.000    2.553    8.016     161.386     1.467   11.5713      3.259         2
  1.000    2.577    7.976     162.090     1.477   11.6501      3.320         2
  1.000    2.754    8.275     179.717     1.499   11.8197      3.792         2

References:
1. L. V. Al'tshuler, G. V. Simakov, R. F. Trunin, To a question on a chemical
   compound of a nucleus of the Earth, Izv. Akad. Nauk SSSR. Fiz. Zemli 1, 3-6
   (1968) [in Russian]
2. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g