Iron-silicon(2.9) alloy, R0 =  7.685 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.988    5.385      40.887     1.225    9.4118      0.488         1
  1.000    1.102    5.572      47.189     1.247    9.5796      0.607         1
  1.000    1.702    6.718      87.871     1.339   10.2926      1.448         1
  1.000    1.703    6.708      87.791     1.340   10.2999      1.450         1
  1.000    2.162    7.516     124.878     1.404   10.7883      2.337         1
  1.000    2.166    7.476     124.443     1.408   10.8198      2.346         1
  1.000    2.259    7.650     132.807     1.419   10.9053      2.552         1
  1.000    2.843    8.666     189.339     1.488   11.4371      4.041         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g