Iron-silicon(3.8) alloy, R0 =  7.652 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.986    5.434      40.999     1.222    9.3482      0.486         1
  1.000    1.094    5.698      47.700     1.238    9.4703      0.598         1
  1.000    1.701    6.753      87.897     1.337   10.2284      1.447         1
  1.000    1.703    6.734      87.753     1.339   10.2422      1.450         1
  1.000    2.165    7.515     124.498     1.405   10.7486      2.344         1
  1.000    2.168    7.493     124.305     1.407   10.7674      2.350         1
  1.000    2.262    7.658     132.551     1.419   10.8597      2.558         1
  1.000    2.308    7.619     134.558     1.435   10.9773      2.663         1
  1.000    2.774    8.585     182.231     1.477   11.3048      3.848         1
  1.000    2.845    8.692     189.224     1.487   11.3753      4.047         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g