Iron-silicon(4.6) alloy, R0 =  7.589 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.984    5.509      41.139     1.217    9.2393      0.484         1
  1.000    1.093    5.753      47.720     1.235    9.3690      0.597         1
  1.000    1.699    6.832      88.090     1.331   10.1009      1.443         1
  1.000    1.706    6.762      87.547     1.337   10.1497      1.455         1
  1.000    2.162    7.608     124.828     1.397   10.6017      2.337         1
  1.000    2.175    7.493     123.680     1.409   10.6928      2.365         1
  1.000    2.271    7.648     131.810     1.422   10.7942      2.579         1
  1.000    2.295    7.794     135.746     1.417   10.7563      2.634         1
  1.000    2.779    8.616     181.710     1.476   11.2021      3.861         1
  1.000    2.857    8.664     187.851     1.492   11.3227      4.081         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g