Iron-silicon(20.0) alloy, R0 =  6.828 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.999    6.783      46.268     1.173    8.0073      0.499         1
  1.000    1.039    6.671      47.326     1.184    8.0876      0.540         1
  1.000    2.687    9.049     166.021     1.422    9.7118      3.610         1
  1.000    2.748    8.921     167.388     1.445    9.8676      3.776         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g