Steel 304, ferritic phase, R0 =  7.805 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.254    4.842       9.599     1.055    8.2371      0.032         1
  1.000    0.706    4.978      27.431     1.165    9.0949      0.249         1
  1.000    1.039    5.616      45.542     1.227    9.5768      0.540         1
  1.000    1.309    6.300      64.366     1.262    9.8520      0.857         1
  1.000    1.769    6.862      94.744     1.347   10.5160      1.565         1
  1.000    2.184    7.629     130.045     1.401   10.9356      2.385         1
  1.000    2.782    8.555     185.759     1.482   11.5662      3.870         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g