Steel 348, R0 =  7.923 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    4.469       0.000     1.000    7.9230      0.000         1
  1.000    0.717    5.605      31.841     1.147    9.0852      0.257         1
  1.000    0.965    6.033      46.127     1.190    9.4316      0.466         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g