Uranium-rhodium(1.0) alloy, R0 = 18.825 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    2.488       0.000     1.000   18.8250      0.000         1
  1.000    0.571    3.372      36.246     1.204   22.6626      0.163         1
  1.000    0.805    3.733      56.570     1.275   24.0006      0.324         1
  1.000    1.191    4.399      98.628     1.371   25.8140      0.709         1
  1.000    1.200    4.324      97.679     1.384   26.0561      0.720         1
  1.000    1.256    4.387     103.727     1.401   26.3766      0.789         1
  1.000    1.710    5.162     166.169     1.495   28.1502      1.462         1
  1.000    1.710    5.170     166.426     1.494   28.1287      1.462         1
  1.000    1.714    5.132     165.589     1.501   28.2650      1.469         1
  1.000    1.720    5.141     166.461     1.503   28.2898      1.479         1
  1.000    1.722    5.126     166.168     1.506   28.3481      1.483         1
  1.000    1.906    5.456     195.764     1.537   28.9322      1.816         1
  1.000    1.910    5.422     194.952     1.544   29.0630      1.824         1
  1.000    1.919    5.421     195.835     1.548   29.1406      1.841         1
  1.000    1.919    5.424     195.943     1.548   29.1318      1.841         1
  1.000    1.923    5.388     195.048     1.555   29.2725      1.849         1
  1.000    1.982    5.566     207.674     1.553   29.2355      1.964         1
  1.000    1.986    5.547     207.383     1.558   29.3239      1.972         1
  1.000    1.991    5.514     206.668     1.565   29.4638      1.982         1
  1.000    2.261    5.986     254.784     1.607   30.2514      2.556         1
  1.000    2.346    6.036     266.571     1.636   30.7934      2.752         1
  1.000    2.350    6.012     265.963     1.642   30.9055      2.761         1
  1.000    2.353    5.985     265.107     1.648   31.0208      2.768         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g