Corundum Mixture, R0 =  3.389 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.573    6.828      36.399     1.299    4.4034      1.237         1
  1.000    1.728    7.107      41.620     1.321    4.4777      1.493         1
  1.000    1.844    7.367      46.039     1.334    4.5205      1.700         1
  1.000    2.066    7.777      54.452     1.362    4.6150      2.134         1
  1.000    2.290    8.167      63.383     1.390    4.7095      2.622         1
  1.000    2.590    8.680      76.189     1.425    4.8303      3.354         1
  1.000    2.866    9.223      89.582     1.451    4.9169      4.107         1
  1.000    3.050    9.412      97.287     1.479    5.0137      4.651         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g