Glass, high-density, Nucleer Pacific x-ray plate, R0 =  4.817 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.397    3.951       7.556     1.112    5.3551      0.079         1
  1.000    0.640    3.658      11.277     1.212    5.8385      0.205         1
  1.000    0.899    3.616      15.659     1.331    6.4108      0.404         1
  1.000    1.165    3.894      21.852     1.427    6.8734      0.679         1
  1.000    1.238    3.866      23.055     1.471    7.0862      0.766         1
  1.000    1.628    4.415      34.623     1.584    7.6308      1.325         1
  1.000    1.671    4.517      36.358     1.587    7.6453      1.396         1
  1.000    1.803    4.703      40.846     1.622    7.8118      1.625         1
  1.000    1.969    4.966      47.101     1.657    7.9817      1.938         1
  1.000    2.150    5.276      54.641     1.688    8.1300      2.311         1
  1.000    2.253    5.465      59.310     1.701    8.1958      2.538         1
  1.000    2.414    5.643      65.618     1.748    8.4182      2.914         1
  1.000    2.623    5.748      72.626     1.839    8.8602      3.440         1
  1.000    2.639    6.005      76.336     1.784    8.5936      3.482         1
  1.000    3.115    6.869     103.069     1.830    8.8141      4.852         1
  1.000    3.155    6.855     104.180     1.853    8.9245      4.977         1
  1.000    3.165    6.788     103.489     1.874    9.0251      5.009         1
  1.000    3.167    6.883     105.003     1.852    8.9223      5.015         1
  1.000    3.258    7.080     111.112     1.852    8.9232      5.307         1
  1.000    3.428    7.361     121.550     1.872    9.0155      5.876         1
  1.000    3.486    7.410     124.429     1.888    9.0963      6.076         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g