Thorium, R0 = 11.680 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.571    2.900      19.341     1.245   14.5436      0.163         1
  1.000    0.620    2.954      21.392     1.266   14.7827      0.192         1
  1.000    0.812    3.192      30.274     1.341   15.6649      0.330         1
  1.000    1.043    3.497      42.601     1.425   16.6442      0.544         1
  1.000    1.900    4.510     100.086     1.728   20.1827      1.805         2
  1.000    1.940    4.530     102.646     1.749   20.4287      1.882         2
  1.000    2.310    5.110     137.872     1.825   21.3160      2.668         2
  1.000    2.320    5.160     139.824     1.817   21.2214      2.691         2
  1.000    2.330    5.090     138.521     1.844   21.5403      2.714         2
  1.000    2.360    5.100     140.581     1.861   21.7401      2.785         2
  1.000    0.000    2.327       0.000     1.000   11.6800      0.000         3
  1.000    0.547    2.865      18.304     1.236   14.4362      0.150         3
  1.000    0.596    2.919      20.320     1.257   14.6767      0.178         3
  1.000    0.787    3.154      28.992     1.332   15.5635      0.310         3
  1.000    1.017    3.455      41.041     1.417   16.5523      0.517         3
  1.000    1.885    4.458      98.151     1.733   20.2369      1.777         3
  1.000    1.920    4.477     100.400     1.751   20.4503      1.843         3
  1.000    2.285    5.048     134.725     1.827   21.3394      2.611         3
  1.000    2.299    5.099     136.920     1.821   21.2701      2.643         3
  1.000    2.303    5.032     135.356     1.844   21.5367      2.652         3
  1.000    2.334    5.041     137.423     1.862   21.7506      2.724         3

References:
1. J. M. Walsh, M. H. Rice, R. G. Mcqueen, F. L. Yarger, Shock-wave compressions
   of twenty-seven metals equations of state of metals, Phys. Rev. 108, 196-216
   (1957)
2. R. G. McQueen, S. P. Marsh, Equation of state for nineteen metallic elements,
   J. Appl. Phys. 31, 1253-1269 (1960)
3. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g