Copper oxide-epoxy mixture, R0 =  1.710 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.284    4.249       9.329     1.433    2.4505      0.824         1
  1.000    1.649    4.850      13.676     1.515    2.5909      1.360         1
  1.000    2.179    5.734      21.366     1.613    2.7581      2.374         1
  1.000    3.730    7.744      49.394     1.929    3.2990      6.956         1
  1.000    3.991    8.198      55.948     1.949    3.3322      7.964         1
  1.000    4.437    8.763      66.487     2.026    3.4639      9.844         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g