Epoxy-lithium aluminum silicate mixture, R0 =  1.775 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.267    4.408       9.913     1.403    2.4910      0.803         1
  1.000    2.194    5.417      21.096     1.681    2.9833      2.407         1
  1.000    3.154    6.821      38.186     1.860    3.3017      4.974         1
  1.000    3.439    6.822      41.643     2.017    3.5794      5.913         1
  1.000    3.958    7.827      54.988     2.023    3.5908      7.833         1
  1.000    4.476    8.348      66.324     2.156    3.8269     10.017         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g