Paraffin-corundum mixture, R0 =  1.662 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.636    3.036       3.209     1.265    2.1024      0.202         1
  1.000    0.932    3.619       5.606     1.347    2.2385      0.434         1
  1.000    1.305    4.253       9.224     1.443    2.3977      0.852         1
  1.000    1.615    4.959      13.311     1.483    2.4647      1.304         1
  1.000    2.204    6.111      22.385     1.564    2.5996      2.429         1
  1.000    2.701    7.089      31.823     1.616    2.6850      3.648         1
  1.000    3.053    7.671      38.923     1.661    2.7608      4.660         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g