Silicon nitride-periclase mixture, R0 =  3.164 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    8.818       0.000     1.000    3.1640      0.000         1
  1.000    2.482    8.787      69.005     1.394    4.4095      3.080         1
  1.000    2.791    9.023      79.680     1.448    4.5810      3.895         1
  1.000    3.333    9.426      99.403     1.547    4.8948      5.554         1
  1.000    3.640    9.725     112.003     1.598    5.0567      6.625         1
  1.000    3.760   10.072     119.823     1.596    5.0488      7.069         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g