Tungsten, syntered-infiltrated copper, Elkonite 10W3, R0 = 14.852 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    3.771       0.000     1.000   14.8520      0.000         1
  1.000    0.189    3.535       9.923     1.056   15.6909      0.018         1
  1.000    0.208    3.616      11.171     1.061   15.7585      0.022         1
  1.000    0.265    3.783      14.889     1.075   15.9708      0.035         1
  1.000    0.288    3.733      15.968     1.084   16.0936      0.041         1
  1.000    0.408    4.024      24.384     1.113   16.5278      0.083         1
  1.000    0.581    4.393      37.907     1.152   17.1156      0.169         1
  1.000    0.818    4.791      58.206     1.206   17.9099      0.335         1
  1.000    0.824    4.723      57.800     1.211   17.9908      0.339         1
  1.000    0.837    4.812      59.819     1.211   17.9793      0.350         1
  1.000    0.875    4.878      63.392     1.219   18.0984      0.383         1
  1.000    1.285    5.534     105.615     1.302   19.3436      0.826         1
  1.000    1.617    5.970     143.374     1.371   20.3690      1.307         1
  1.000    1.836    6.259     170.672     1.415   21.0171      1.685         1
  1.000    2.128    6.648     210.111     1.471   21.8443      2.264         1
  1.000    2.191    6.722     218.739     1.484   22.0338      2.400         1
  1.000    2.237    6.739     223.896     1.497   22.2318      2.502         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g