Tungsten, syntered-infiltrated copper, Elkonite 3W3, R0 = 13.812 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    3.785       0.000     1.000   13.8120      0.000         1
  1.000    0.533    4.354      32.053     1.139   15.7387      0.142         1
  1.000    1.073    5.177      76.725     1.261   17.4232      0.576         1
  1.000    1.568    6.017     130.312     1.352   18.6799      1.229         1
  1.000    2.436    7.203     242.352     1.511   20.8701      2.967         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g