Tungsten, syntered-infiltrated copper, Elkonite 1W3, R0 = 12.315 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    3.357       0.000     1.000   12.3150      0.000         1
  1.000    0.341    3.668      15.404     1.102   13.5772      0.058         1
  1.000    0.436    3.831      20.570     1.128   13.8965      0.095         1
  1.000    0.513    4.086      25.814     1.144   14.0831      0.132         1
  1.000    0.576    4.214      29.892     1.158   14.2648      0.166         1
  1.000    0.681    4.416      37.035     1.182   14.5604      0.232         1
  1.000    0.804    4.442      43.981     1.221   15.0366      0.323         1
  1.000    0.878    4.729      51.133     1.228   15.1227      0.385         1
  1.000    1.047    5.028      64.830     1.263   15.5538      0.548         1
  1.000    1.158    5.184      73.928     1.288   15.8572      0.670         1
  1.000    1.304    5.434      87.263     1.316   16.2033      0.850         1
  1.000    1.339    5.311      87.577     1.337   16.4665      0.896         1
  1.000    1.479    5.652     102.945     1.354   16.6797      1.094         1
  1.000    1.533    5.785     109.215     1.361   16.7550      1.175         1
  1.000    1.590    5.897     115.468     1.369   16.8613      1.264         1
  1.000    2.031    6.496     162.477     1.455   17.9167      2.062         1
  1.000    2.263    6.792     189.285     1.500   18.4684      2.561         1
  1.000    2.485    7.216     220.830     1.525   18.7836      3.088         1
  1.000    2.564    7.307     230.723     1.541   18.9723      3.287         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g