Tungsten carbide, syntered-infiltrated copper, Elkonite TC10, R0 = 11.653 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    4.203       0.000     1.000   11.6530      0.000         1
  1.000    0.198    4.135       9.541     1.050   12.2391      0.020         1
  1.000    0.216    4.296      10.813     1.053   12.2699      0.023         1
  1.000    0.279    4.364      14.188     1.068   12.4489      0.039         1
  1.000    0.305    4.330      15.390     1.076   12.5360      0.047         1
  1.000    0.429    4.649      23.241     1.102   12.8376      0.092         1
  1.000    0.619    4.934      35.590     1.143   13.3247      0.192         1
  1.000    0.936    5.416      59.074     1.209   14.0876      0.438         1
  1.000    1.377    6.086      97.657     1.292   15.0606      0.948         1
  1.000    1.723    6.609     132.696     1.353   15.7623      1.484         1
  1.000    1.954    6.961     158.502     1.390   16.2006      1.909         1
  1.000    2.261    7.383     194.523     1.441   16.7970      2.556         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g