Tungsten carbide, syntered-infiltrated silver, Elkonite G-12, R0 = 11.936 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    3.572       0.000     1.000   11.9360      0.000         1
  1.000    0.632    4.251      32.068     1.175   14.0204      0.200         1
  1.000    1.353    5.602      90.469     1.318   15.7368      0.915         1
  1.000    1.639    6.185     120.998     1.361   16.2394      1.343         1
  1.000    2.489    7.324     217.587     1.515   18.0805      3.098         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g