Periclase-corundum mixture, R0 =  2.118 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.661    3.740      13.157     1.799    3.8102      1.379         1
  1.000    2.145    4.953      22.502     1.764    3.7359      2.301         1
  1.000    2.489    5.219      27.513     1.912    4.0490      3.098         1
  1.000    2.741    5.851      33.968     1.881    3.9847      3.757         1
  1.000    2.992    6.432      40.760     1.870    3.9602      4.476         1
  1.000    3.040    6.764      43.552     1.816    3.8470      4.621         1
  1.000    3.133    6.711      44.532     1.876    3.9726      4.908         1
  1.000    3.465    7.098      52.091     1.954    4.1381      6.003         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g