Periclase-quartz(33) mixture, R0 =  1.894 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.339    3.067       7.778     1.775    3.3616      0.896         1
  1.000    1.825    4.003      13.837     1.838    3.4810      1.665         1
  1.000    2.309    4.604      20.135     2.006    3.7996      2.666         1
  1.000    2.372    4.711      21.165     2.014    3.8147      2.813         1
  1.000    2.508    5.078      24.121     1.976    3.7423      3.145         1
  1.000    2.666    5.071      25.606     2.109    3.9935      3.554         1
  1.119    1.773    3.596      10.794     1.763    3.3396      1.572         1
  1.119    2.361    4.389      17.544     1.935    3.6640      2.787         1
  1.119    2.691    4.937      22.492     1.965    3.7214      3.621         1
  1.119    2.976    5.493      27.676     1.951    3.6947      4.428         1
  1.119    3.278    5.988      33.231     1.975    3.7408      5.373         1
  1.119    3.358    6.198      35.236     1.951    3.6948      5.638         1
  1.119    3.429    6.288      36.504     1.966    3.7235      5.879         1
  1.119    3.771    6.821      43.547     1.999    3.7862      7.110         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g