Niobium(95)-tantalum(5) alloy, R0 =  8.790 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.940    5.570      46.023     1.203   10.5746      0.442         1
  1.000    1.800    6.570     103.951     1.377   12.1070      1.620         1
  1.000    2.420    7.270     154.646     1.499   13.1759      2.928         1
  1.000    2.900    8.070     205.712     1.561   13.7206      4.205         1
  1.000    4.480   10.230     402.849     1.779   15.6386     10.035         1

References:
1. A. A. Bakanova, I. P. Dudoladov, Yu. N. Sutulov, Fulfillment of additive law
   for shock-compressed alloys, Zh. Prikl. Mekh. Tekhn. Fiz. 6, 167-172 (1972)
   [in Russian] (J. Appl. Mech. Techn. Phys. 13 (1972))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g