Zinc, liquid, To=723 K, R0 =  6.560 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.750    3.940      19.385     1.235    8.1023      0.281         1
  1.000    0.970    4.530      28.825     1.272    8.3474      0.470         1
  1.000    1.540    5.110      51.623     1.431    9.3898      1.186         1
  1.000    2.040    6.010      80.428     1.514    9.9309      2.081         1
  1.000    2.750    7.170     129.347     1.622   10.6414      3.781         1
  1.000    3.070    7.840     157.891     1.644   10.7821      4.712         1

References:
1. R. F. Trunin, M. V. Zhernokletov, N. F. Kuznetsov, V. V. Shutov, Dynamical
   compressibility of melted and cooled metals, Teplofiz. Vys. Temp. 33(2),
   222-226 (1995) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g