Silicon, R0 =  2.360 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    4.020    8.740      82.918     1.852    4.3700      8.080         1
  1.000    4.130    8.900      86.747     1.866    4.4034      8.528         1
  1.000    4.980   10.450     122.817     1.910    4.5086     12.400         1
  1.000    6.380   13.000     195.738     1.964    4.6344     20.352         1

References:
1. M. N. Pavlovskii, Formation of metallic modifications of germanium and silicon
   under conditions of shock compression, Fiz. Tverd. Tela 9(11), 3192-3197
   (1967) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g