Copper-carbide (diamond) mixture, R0 =  6.220 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.194    2.240    7.050      82.276     1.228    7.6363      2.509         1
  1.203    1.770    5.940      54.356     1.184    7.3645      1.566         1
  1.208    0.870    3.750      16.802     1.078    6.7057      0.378         1
  1.224    3.060    8.840     137.416     1.249    7.7694      4.682         1
  1.234    1.100    4.150      23.008     1.103    6.8577      0.605         1
  1.234    2.730    7.950     109.386     1.234    7.6759      3.726         1
  1.502    1.330    3.420      18.831     1.089    6.7745      0.884         1
  1.616    2.170    5.020      41.940     1.090    6.7814      2.354         1
  1.641    2.730    6.250      64.667     1.082    6.7294      3.726         1
  1.668    1.130    2.740      11.549     1.021    6.3480      0.638         1
  1.690    3.600    8.050     106.647     1.070    6.6571      6.480         1

References:
1. R. F. Trunin, L.F.Gudarenko, M. V. Zhernokletov, G. V. Simakov, Experimental
   data on shock compressibility and adiabatic expansion of condensed substances,
   RFNC, Sarov (2001) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g