Feldspar-paraffin mixture, R0 =  1.890 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.030    4.560       8.877     1.292    2.4415      0.530    1    1
  1.011    1.170    4.770      10.436     1.311    2.4778      0.684    1    1
  1.011    1.390    4.950      12.867     1.376    2.6001      0.966    1    1
  1.022    1.840    5.400      18.382     1.485    2.8062      1.693    2    1
  1.022    2.400    6.190      27.484     1.599    3.0215      2.880    2    1

References:
1. G. A. Adadurov, A. N. Dremin, Yu. N. Ryabinin, About behaviour of some
   substances at shock compression, Zh. Prikl. Mekh. Tekhn. Fiz. 4, 115-119
   (1964) [in Russian]

Remarks:
1. Feldstar content 80.8%
2. Feldstar content 79.0%

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g