Silicon nitride, R0 =  3.440 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.121    0.980    8.570      25.784     1.008    3.4664      0.480         1
  1.121    1.290    8.620      34.138     1.050    3.6103      0.832         1
  1.121    1.880    8.800      50.790     1.135    3.9040      1.767         1
  1.121    2.610    8.850      70.912     1.266    4.3541      3.406         1
  1.121    2.810    8.960      77.295     1.300    4.4727      3.948         1
  1.121    3.250    9.280      92.591     1.373    4.7246      5.281         1
  1.121    3.700   10.080     114.499     1.410    4.8504      6.845         1
  1.121    3.960    8.260     100.419     1.714    5.8973      7.841         1

References:
1. A. A. Bakanova, V. A. Bugaeva, I. P. Dudoladov, R. F. Trunin, Shock
   compressibility of nitrides and carbides of metalls, Fiz. Zemli. 6, 58-63
   (1995) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g