Magnesium hidride, R0 =  1.420 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.036    3.800    8.600      44.772     1.729    2.4546      7.220         1
  1.036    4.240    9.300      54.022     1.773    2.5180      8.989         1
  1.036    4.720    9.940      64.276     1.837    2.6088     11.139         1
  1.036    5.160   10.520      74.368     1.894    2.6889     13.313         1
  1.044    1.560    5.730      12.157     1.316    1.8688      1.217         1
  1.044    2.430    6.720      22.208     1.500    2.1303      2.952         1
  1.044    6.900   13.020     122.180     2.038    2.8933     23.805         1
  1.052    1.070    5.100       7.367     1.203    1.7084      0.572         1
  1.052    2.000    6.110      16.497     1.413    2.0069      2.000         1
  1.060    2.870    7.030      27.036     1.595    2.2645      4.118         1
  1.060    3.550    8.250      39.245     1.656    2.3521      6.301         1

References:
1. R. F. Trunin, M. V. Zhernokletov, N. F. Kuznetsov, Yu. N. Sutulov, Shock
   compressibility of hydrides of metalls, Fiz. Zemli. 11, 65-70 (1987) [in
   Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g